Examples of Steel Fractography

Download Report

Transcript Examples of Steel Fractography

Examples of Steel Fractography
Professor M Neil James
mjames@plymouth.ac.uk
Department of Mechanical & Marine Engineering
University of Plymouth
Drake Circus, Plymouth PL4 8AA
ENGLAND
1
Fractography Resource - mjames@plymouth.ac.uk
Contents – Use the hyperlinks to navigate around this resource

Fatigue crack growth in moist air

Fatigue crack growth in vacuum

Crack growth by hydrogen embrittlement

Low carbon interstitial-free steels

Charpy impact fracture

Fatigue in a high tensile bolt
2
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in Air
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Quenched & Tempered - YS = 653 MPa – Grain size 10m – vestigial
striations present
Linear growth rate
regime ~ 10-4
mm/cycle
Original
magnification 2kx
3
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in Air
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Quenched & Tempered - YS = 653 MPa – Grain size 10m – vestigial
striations present
Linear growth rate
regime ~ 10-4
mm/cycle
Original
magnification 5kx
4
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in Air
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Quenched & Tempered - YS = 653 MPa – Grain size 10m – ductile
transgranular with some evidence of underlying structure
Threshold growth
rate regime ~ 10-7
mm/cycle
Original
magnification 2kx
5
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in Air
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Quenched & Tempered - YS = 653 MPa – Grain size 10m – ductile
transgranular with some evidence of underlying structure
Threshold growth
rate regime ~ 10-7
mm/cycle
Original
magnification 5kx
6
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in Air
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Quenched & Tempered - YS = 653 MPa – Grain size 10m – ductile
transgranular
Threshold growth
rate regime ~ 10-7
mm/cycle
Original
magnification 2kx
7
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in Air
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Quenched & Tempered - YS = 653 MPa – Grain size 10m – ductile
transgranular with some environment (moisture) induced IG facets
'Knee' of growth rate
regime ~ 10-6
mm/cycle
Original
magnification 2kx
8
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in Air
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Quenched & Tempered - YS = 653 MPa – Grain size 10m – ductile
transgranular with some moisture-induced oxide build-up by fretting
'Knee' of growth rate
regime ~ 10-6
mm/cycle
Original
magnification 1.15kx
Mechanism of oxideinduced fatigue
crack closure
9
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in Air
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Quenched & Tempered - YS = 653 MPa – Grain size 10m – ductile
transgranular with some moisture-induced oxide build-up by fretting
'Knee' of growth rate
regime ~ 10-6
mm/cycle
Original
magnification 7.6kx
Mechanism of oxideinduced fatigue
crack closure
10
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in Air
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Q&T CGHAZ simulation – Grain size 58m – microstructure has bigger
influence (e.g. bainite packets) – clear IG facets
Threshold growth
rate regime < 10-6
mm/cycle
Original
magnification 500x
11
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in Air
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Q&T CGHAZ simulation – Grain size 58m – microstructure has bigger
influence (e.g. bainite packets) – clear IG facets
Threshold growth
rate regime < 10-6
mm/cycle
Original
magnification 500x
12
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in Air
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Q&T CGHAZ simulation – Grain size 58m – microstructure has bigger
influence (e.g. bainite packets) – ductile transgranular
Threshold growth
rate regime < 10-6
mm/cycle
Original
magnification 2kx
Back to Contents
13
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in Vacuum
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Q&T CGHAZ simulation – Grain size 58m – no 'knee' in da/dN curve,
implying no mechanism change over range of growth rate 10-4 to 10-7
mm/cycle. No IG facets in absence of moist air
Growth rate ~ 10-4
mm/cycle
Original
magnification 500x
14
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in Vacuum
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Q&T CGHAZ simulation – Grain size 58m – no 'knee' in da/dN curve,
implying no mechanism change over range of growth rate 10-4 to 10-7
mm/cycle. No IG facets in absence of moist air
Growth rate ~ 10-4
mm/cycle
Original
magnification 2kx
15
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in Vacuum
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Q&T CGHAZ simulation – Grain size 58m – no 'knee' in da/dN curve,
implying no mechanism change over range of growth rate 10-4 to 10-7
mm/cycle. No IG facets in absence of moist air
Growth rate ~ 10-7
mm/cycle
Original
magnification 500x
16
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in Vacuum
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Q&T CGHAZ simulation – Grain size 58m – no 'knee' in da/dN curve,
implying no mechanism change over range of growth rate 10-4 to 10-7
mm/cycle. No IG facets in absence of moist air
Growth rate ~ 10-7
mm/cycle
Original
magnification 2kx
17
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in Vacuum
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Q&T - Grain size 10m – no 'knee' in da/dN curve, implying no
mechanism change over range of growth rate 10-4 to 10-7 mm/cycle. No
IG facets in absence of moist air
Growth rate ~ 10-7
mm/cycle
Original
magnification 2kx
18
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in Vacuum
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Q&T - Grain size 10m – no 'knee' in da/dN curve, implying no
mechanism change over range of growth rate 10-4 to 10-7 mm/cycle. No
IG facets in absence of moist air
Growth rate ~ 10-7
mm/cycle
Original
magnification 5kx
Back to Contents
19
Fractography Resource - mjames@plymouth.ac.uk
Crack Growth by Hydrogen Embrittlement
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Q&T - Grain size 10m – Hydrogen can cause cleavage, quasi-cleavage,
MVC or IG fracture, depending on crack tip stress, H2 concentration and
its effect on plasticity
Quasi-cleavage at
initiation site
changes to IG as
crack tip stress
decreases
Bend loading + H2
charging
Original
magnification given
by micron bar
20
Fractography Resource - mjames@plymouth.ac.uk
Crack Growth by Hydrogen Embrittlement
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Q&T - Grain size 10m – Hydrogen can cause cleavage, quasi-cleavage,
MVC or IG fracture, depending on crack tip stress, H2 concentration and
its effect on plasticity
Quasi-cleavage at
initiation site shown
at higher
magnification
Bend loading + H2
charging
Original
magnification given
by micron bar
21
Fractography Resource - mjames@plymouth.ac.uk
Crack Growth by Hydrogen Embrittlement
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Q&T - Grain size 10m – Hydrogen can cause cleavage, quasi-cleavage,
MVC or IG fracture, depending on crack tip stress, H2 concentration and
its effect on plasticity
Quasi-cleavage at
initiation site
changes to IG as
crack tip stress
decreases
Bend loading + H2
charging
Original
magnification given
by micron bar
22
Fractography Resource - mjames@plymouth.ac.uk
Crack Growth by Hydrogen Embrittlement
Q1N Steel (HY 80) – 0.2C 2.5Ni 1.5Cr 0.5 Mo
Q&T - Grain size 10m – Comparison between IG and cleavage (induced
by fracture at cryogenic temperatures)
IG region is on the
left, and cleavage is
on the right. Line
demarcates the
boundary.
Original
magnification given
by micron bar
Back to Contents
23
Fractography Resource - mjames@plymouth.ac.uk
Low Carbon Interstitial-Free Steel
Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa
Some of these steels show IG fatigue at low levels of plasticity (e.g. during
crack initiation, and at long lives)
Nf = 1 196 172
cycles
Fatigue performance
is no worse than
grades that do not
show IG fatigue
Original
magnification given
by micron bar
24
Fractography Resource - mjames@plymouth.ac.uk
Low Carbon Interstitial-Free Steel
Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa
Some of these steels show IG fatigue at low levels of plasticity (e.g. during
crack initiation, and at long lives)
Nf = 1 196 172
cycles
Fatigue striations on
an IG facet
Original
magnification given
by micron bar
25
Fractography Resource - mjames@plymouth.ac.uk
Low Carbon Interstitial-Free Steel
Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa
Some of these steels show IG fatigue at low levels of plasticity (e.g. during
crack initiation, and at long lives)
Nf = 1 196 172
cycles
Fatigue striations on
IG facets
Original
magnification given
by micron bar
26
Fractography Resource - mjames@plymouth.ac.uk
Low Carbon Interstitial-Free Steel
Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa
Some of these steels show IG fatigue at low levels of plasticity (e.g. during
crack initiation, and at long lives)
Nf = 1 196 172
cycles
IG facets at crack
initiation site
Original
magnification given
by micron bar
27
Fractography Resource - mjames@plymouth.ac.uk
Low Carbon Interstitial-Free Steel
Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa
Some of these steels show IG fatigue at low levels of plasticity (e.g. during
crack initiation, and at long lives)
Nf = 24 371 cycles
IG facets at crack
initiation site
(although damaged
by surface contact)
Original
magnification given
by micron bar
28
Fractography Resource - mjames@plymouth.ac.uk
Low Carbon Interstitial-Free Steel
Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa
Some of these steels show IG fatigue at low levels of plasticity (e.g. during
crack initiation, and at long lives)
Nf = 24 371 cycles
Striation growth
once crack is
established and
plasticity levels are
higher at crack tip
Original
magnification given
by micron bar
29
Fractography Resource - mjames@plymouth.ac.uk
Low Carbon Interstitial-Free Steel
Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa
Some of these steels show IG fatigue at low levels of plasticity (e.g. during
crack initiation, and at long lives)
Nf = 24 371 cycles
Fatigue striations at
higher magnification
Original
magnification given
by micron bar
30
Fractography Resource - mjames@plymouth.ac.uk
Low Carbon Interstitial-Free Steel
Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa
An extra-low carbon grade does not show IG fatigue
Nf = 37 782 cycles
No IG facets near
crack initiation site
Original
magnification given
by micron bar
31
Fractography Resource - mjames@plymouth.ac.uk
Low Carbon Interstitial-Free Steel
Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa
An extra-low carbon grade does not show IG fatigue
Nf = 37 782 cycles
Higher magnification
view of crack
initiation site
Original
magnification given
by micron bar
Back to Contents
32
Fractography Resource - mjames@plymouth.ac.uk
Charpy Impact Fracture
Plain medium carbon steel (0.4%C) with a normalised microstructure
Low temperature
fracture showing
cleavage
Original
magnification given
by micron bar
33
Fractography Resource - mjames@plymouth.ac.uk
Charpy Impact Fracture
Plain medium carbon steel (0.4%C) with a normalised microstructure
Low temperature
fracture showing
cleavage – twist and
tilt grain boundaries
evident
Original
magnification given
by micron bar
34
Fractography Resource - mjames@plymouth.ac.uk
Charpy Impact Fracture
Plain medium carbon steel (0.4%C) with a normalised microstructure
Ductile fracture at
room temperature
showing MVC
Original
magnification given
by micron bar
35
Fractography Resource - mjames@plymouth.ac.uk
Charpy Impact Fracture
Plain medium carbon steel (0.4%C) with a normalised microstructure
Room temperature
fracture showing
MVC and regions of
brittle inter-pearlitic
fracture
Original
magnification given
by micron bar
36
Fractography Resource - mjames@plymouth.ac.uk
Charpy Impact Fracture
Plain medium carbon steel (0.4%C) with a normalised microstructure
Room temperature
fracture showing
MVC at high
magnification with
inclusion in hole
Original
magnification given
by micron bar
37
Fractography Resource - mjames@plymouth.ac.uk
Charpy Impact Fracture
Plain medium carbon steel (0.4%C) with a normalised microstructure
Shear micro-voids
can occur where
plastic constraint is
lower, towards the
specimen edges
Original
magnification given
by micron bar
38
Fractography Resource - mjames@plymouth.ac.uk
Charpy Impact Fracture
Plain medium carbon steel (0.4%C) with a normalised microstructure
Smooth featureless
shear can also occur
at specimen edges
Original
magnification given
by micron bar
Back to Contents
39
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in a High Tensile Bolt
High tensile bolt with Q&T microstructure
Fatigue in bend with
a slightly reversed
component
Original
magnification given
by micron bar
Back to Contents
40
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in a High Tensile Bolt
High tensile bolt with Q&T microstructure
Clear striations are
present in this low
cycle fatigue
situation; this is the
reversed bend area.
Original
magnification given
by micron bar
Back to Contents
41
Fractography Resource - mjames@plymouth.ac.uk
Fatigue in a High Tensile Bolt
High tensile bolt with Q&T microstructure
High magnification
view of fatigue
striations in the main
fatigue region.
Original
magnification given
by micron bar
Back to Contents
42
Fractography Resource - mjames@plymouth.ac.uk